EN AW-6082
Round bar
 
                                    - Form Round bar
- Material Aluminum
- Material EN AW-6082
- Material chemically EN 573-3 AlSi1MgMn
- DIN 3.2315
 
             
            BIKAR Metals companies
 
                                     
             
            Shipbuilding
Railed vehicles
Boiler and container construction
Machine construction
| Aviation | No | 
| Cr (to) | 0,25 | 
| Cu (to) | 0,1 | 
| Fe (to) | 0,5 | 
| Mg (from) | 0,6 | 
| Mg (to) | 1,2 | 
| Mn (from) | 0,4 | 
| Mn (to) | 1 | 
| Other | 0,05 | 
| Rest | Aluminium | 
| Si (from) | 0,7 | 
| Si (to) | 1,3 | 
| Ti (to) | 0,1 | 
| Total | 0,15 | 
| Zn (to) | 0,2 | 
(a) Includes all listed elements for which no limits are specified. (b) The sum of these "other impurities" whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
| Anodise - decorative | 3 | 
| Anodising - protective anodising | 1 | 
| Normal atmosphere | 1 | 
| Seawater atmosphere | 2 | 
| suitable according to DIN EN 602 | Yes | 
| Bending | 3 | 
| Bending delivery conditions | T3 · T4 | 
| Deep drawing (conditional) | 2 | 
| Deep drawing conditions | O | 
| Drop forging | 2 | 
| Extruding | 2 | 
| Impact extrusion | 2 | 
| Impact extrusion conditions | O | 
| Open die forging | 2 | 
| Press | 2 | 
| Press conditions | O | 
| Upsetting (Conditional) | 2 | 
| Upsetting conditions | O | 
| Heating time max. | 2 h | 
| Heating time min. | 1 h | 
| Annealing temperature max. | 420 °C | 
| Annealing temperature min. | 380 °C | 
| Cooling conditions | ≤ 30°C/h up to 250°C, below 250°C in the air | 
| Cold ageing max. | 8 d | 
| Cold ageing min. | 5 d | 
| Heat ageing max. | 16 h | 
| Heat ageing min. | 4 h | 
| Heating temperature max. | 190 °C | 
| Heating temperature min. | 155 °C | 
| Quenching | Water, Air | 
| Solution annealing max. | 540 °C | 
| Solution annealing min. | 525 °C | 
| dimensional stability | 3 | 
| Eroding | 1 | 
| hardened | 2 | 
| soft annealed | 4 | 
| Colorcode | Enzianblau (RAL 5010) | 
| Material chemically EN 573-3 | AlSi1MgMn | 
| DIN | 3,2315 | 
| DIN (old designation) | Al Mg Si1 | 
| France AFNOR | A-SGM0,7 | 
| Italy UNI | 9006/4 | 
| Material no | EN AW-6082 | 
| Norway | - | 
| Spain | L-3453 | 
| Sweden | 144.212 | 
| United Kingdom BS | H30 | 
| Polishing | 1 | 
| Painting / Coating | 2 | 
| Coefficient of thermal expansion from 20 to 100°C | 23.4 K⁻¹10⁻⁶ | 
| Density | 2.7 g/cm³ | 
| Electrical conductivity max. | 32 m/Ω*mm² | 
| Electrical conductivity min. | 24 m/Ω*mm² | 
| Modulus of elasticity | 70 GPa | 
| Shear modulus | 26.4 GPa | 
| Specific heat | 896 J/(kg·K) | 
| Thermal conductivity max. | 220 W/m*K | 
| Thermal conductivity min. | 170 W/m*K | 
| Brazing | 4 | 
| Brazing with flux | 3 | 
| Friction soldering | 2 | 
| Soft soldering with flux | 3 | 
| Gas | 3 | 
| MIG | 1 | 
| Resistance spot welding | 3 | 
| TIG | 2 | 
| welding additives | 
 | 
| Aviation | No | 
| Cr (to) | 0,25 | 
| Cu (to) | 0,1 | 
| Fe (to) | 0,5 | 
| Mg (from) | 0,6 | 
| Mg (to) | 1,2 | 
| Mn (from) | 0,4 | 
| Mn (to) | 1 | 
| Other | 0,05 | 
| Rest | Aluminium | 
| Si (from) | 0,7 | 
| Si (to) | 1,3 | 
| Ti (to) | 0,1 | 
| Total | 0,15 | 
| Zn (to) | 0,2 | 
(a) Includes all listed elements for which no limits are specified. (b) The sum of these "other impurities" whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
| Anodise - decorative | 3 | 
| Anodising - protective anodising | 1 | 
| Normal atmosphere | 1 | 
| Seawater atmosphere | 2 | 
| suitable according to DIN EN 602 | Yes | 
| Bending | 3 | 
| Bending delivery conditions | T3 · T4 | 
| Deep drawing (conditional) | 2 | 
| Deep drawing conditions | O | 
| Drop forging | 2 | 
| Extruding | 2 | 
| Impact extrusion | 2 | 
| Impact extrusion conditions | O | 
| Open die forging | 2 | 
| Press | 2 | 
| Press conditions | O | 
| Upsetting (Conditional) | 2 | 
| Upsetting conditions | O | 
| Heating time max. | 2 h | 
| Heating time min. | 1 h | 
| Annealing temperature max. | 420 °C | 
| Annealing temperature min. | 380 °C | 
| Cooling conditions | ≤ 30°C/h up to 250°C, below 250°C in the air | 
| Cold ageing max. | 8 d | 
| Cold ageing min. | 5 d | 
| Heat ageing max. | 16 h | 
| Heat ageing min. | 4 h | 
| Heating temperature max. | 190 °C | 
| Heating temperature min. | 155 °C | 
| Quenching | Water, Air | 
| Solution annealing max. | 540 °C | 
| Solution annealing min. | 525 °C | 
| dimensional stability | 3 | 
| Eroding | 1 | 
| hardened | 2 | 
| soft annealed | 4 | 
| Colorcode | Enzianblau (RAL 5010) | 
| Material chemically EN 573-3 | AlSi1MgMn | 
| DIN | 3,2315 | 
| DIN (old designation) | Al Mg Si1 | 
| France AFNOR | A-SGM0,7 | 
| Italy UNI | 9006/4 | 
| Material no | EN AW-6082 | 
| Norway | - | 
| Spain | L-3453 | 
| Sweden | 144.212 | 
| United Kingdom BS | H30 | 
| Polishing | 1 | 
| Painting / Coating | 2 | 
| Coefficient of thermal expansion from 20 to 100°C | 23.4 K⁻¹10⁻⁶ | 
| Density | 2.7 g/cm³ | 
| Electrical conductivity max. | 32 m/Ω*mm² | 
| Electrical conductivity min. | 24 m/Ω*mm² | 
| Modulus of elasticity | 70 GPa | 
| Shear modulus | 26.4 GPa | 
| Specific heat | 896 J/(kg·K) | 
| Thermal conductivity max. | 220 W/m*K | 
| Thermal conductivity min. | 170 W/m*K | 
| Brazing | 4 | 
| Brazing with flux | 3 | 
| Friction soldering | 2 | 
| Soft soldering with flux | 3 | 
| Gas | 3 | 
| MIG | 1 | 
| Resistance spot welding | 3 | 
| TIG | 2 | 
| welding additives | 
 | 
| Aviation | No | 
| Cr (to) | 0,25 | 
| Cu (to) | 0,1 | 
| Fe (to) | 0,5 | 
| Mg (from) | 0,6 | 
| Mg (to) | 1,2 | 
| Mn (from) | 0,4 | 
| Mn (to) | 1 | 
| Other | 0,05 | 
| Rest | Aluminium | 
| Si (from) | 0,7 | 
| Si (to) | 1,3 | 
| Ti (to) | 0,1 | 
| Total | 0,15 | 
| Zn (to) | 0,2 | 
(a) Includes all listed elements for which no limits are specified. (b) The sum of these "other impurities" whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
| Anodise - decorative | 3 | 
| Anodising - protective anodising | 1 | 
| Normal atmosphere | 1 | 
| Seawater atmosphere | 2 | 
| suitable according to DIN EN 602 | Yes | 
| Bending | 3 | 
| Bending delivery conditions | T3 · T4 | 
| Deep drawing (conditional) | 2 | 
| Deep drawing conditions | O | 
| Drop forging | 2 | 
| Extruding | 2 | 
| Impact extrusion | 2 | 
| Impact extrusion conditions | O | 
| Open die forging | 2 | 
| Press | 2 | 
| Press conditions | O | 
| Upsetting (Conditional) | 2 | 
| Upsetting conditions | O | 
| Heating time max. | 2 h | 
| Heating time min. | 1 h | 
| Annealing temperature max. | 420 °C | 
| Annealing temperature min. | 380 °C | 
| Cooling conditions | ≤ 30°C/h up to 250°C, below 250°C in the air | 
| Cold ageing max. | 8 d | 
| Cold ageing min. | 5 d | 
| Heat ageing max. | 16 h | 
| Heat ageing min. | 4 h | 
| Heating temperature max. | 190 °C | 
| Heating temperature min. | 155 °C | 
| Quenching | Water, Air | 
| Solution annealing max. | 540 °C | 
| Solution annealing min. | 525 °C | 
| dimensional stability | 3 | 
| Eroding | 1 | 
| hardened | 2 | 
| soft annealed | 4 | 
| Colorcode | Enzianblau (RAL 5010) | 
| Material chemically EN 573-3 | AlSi1MgMn | 
| DIN | 3,2315 | 
| DIN (old designation) | Al Mg Si1 | 
| France AFNOR | A-SGM0,7 | 
| Italy UNI | 9006/4 | 
| Material no | EN AW-6082 | 
| Norway | - | 
| Spain | L-3453 | 
| Sweden | 144.212 | 
| United Kingdom BS | H30 | 
| Polishing | 1 | 
| Painting / Coating | 2 | 
| Coefficient of thermal expansion from 20 to 100°C | 23.4 K⁻¹10⁻⁶ | 
| Density | 2.7 g/cm³ | 
| Electrical conductivity max. | 32 m/Ω*mm² | 
| Electrical conductivity min. | 24 m/Ω*mm² | 
| Modulus of elasticity | 70 GPa | 
| Shear modulus | 26.4 GPa | 
| Specific heat | 896 J/(kg·K) | 
| Thermal conductivity max. | 220 W/m*K | 
| Thermal conductivity min. | 170 W/m*K | 
| Brazing | 4 | 
| Brazing with flux | 3 | 
| Friction soldering | 2 | 
| Soft soldering with flux | 3 | 
| Gas | 3 | 
| MIG | 1 | 
| Resistance spot welding | 3 | 
| TIG | 2 | 
| welding additives | 
 | 
| Aviation | No | 
| Cr (to) | 0,25 | 
| Cu (to) | 0,1 | 
| Fe (to) | 0,5 | 
| Mg (from) | 0,6 | 
| Mg (to) | 1,2 | 
| Mn (from) | 0,4 | 
| Mn (to) | 1 | 
| Other | 0,05 | 
| Rest | Aluminium | 
| Si (from) | 0,7 | 
| Si (to) | 1,3 | 
| Ti (to) | 0,1 | 
| Total | 0,15 | 
| Zn (to) | 0,2 | 
(a) Includes all listed elements for which no limits are specified. (b) The sum of these "other impurities" whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
| Anodise - decorative | 3 | 
| Anodising - protective anodising | 1 | 
| Normal atmosphere | 1 | 
| Seawater atmosphere | 2 | 
| suitable according to DIN EN 602 | Yes | 
| Bending | 3 | 
| Bending delivery conditions | T3 · T4 | 
| Deep drawing (conditional) | 2 | 
| Deep drawing conditions | O | 
| Drop forging | 2 | 
| Extruding | 2 | 
| Impact extrusion | 2 | 
| Impact extrusion conditions | O | 
| Open die forging | 2 | 
| Press | 2 | 
| Press conditions | O | 
| Upsetting (Conditional) | 2 | 
| Upsetting conditions | O | 
| Heating time max. | 2 h | 
| Heating time min. | 1 h | 
| Annealing temperature max. | 420 °C | 
| Annealing temperature min. | 380 °C | 
| Cooling conditions | ≤ 30°C/h up to 250°C, below 250°C in the air | 
| Cold ageing max. | 8 d | 
| Cold ageing min. | 5 d | 
| Heat ageing max. | 16 h | 
| Heat ageing min. | 4 h | 
| Heating temperature max. | 190 °C | 
| Heating temperature min. | 155 °C | 
| Quenching | Water, Air | 
| Solution annealing max. | 540 °C | 
| Solution annealing min. | 525 °C | 
| dimensional stability | 3 | 
| Eroding | 1 | 
| hardened | 2 | 
| soft annealed | 4 | 
| Colorcode | Enzianblau (RAL 5010) | 
| Material chemically EN 573-3 | AlSi1MgMn | 
| DIN | 3,2315 | 
| DIN (old designation) | Al Mg Si1 | 
| France AFNOR | A-SGM0,7 | 
| Italy UNI | 9006/4 | 
| Material no | EN AW-6082 | 
| Norway | - | 
| Spain | L-3453 | 
| Sweden | 144.212 | 
| United Kingdom BS | H30 | 
| Polishing | 1 | 
| Painting / Coating | 2 | 
| Coefficient of thermal expansion from 20 to 100°C | 23.4 K⁻¹10⁻⁶ | 
| Density | 2.7 g/cm³ | 
| Electrical conductivity max. | 32 m/Ω*mm² | 
| Electrical conductivity min. | 24 m/Ω*mm² | 
| Modulus of elasticity | 70 GPa | 
| Shear modulus | 26.4 GPa | 
| Specific heat | 896 J/(kg·K) | 
| Thermal conductivity max. | 220 W/m*K | 
| Thermal conductivity min. | 170 W/m*K | 
| Brazing | 4 | 
| Brazing with flux | 3 | 
| Friction soldering | 2 | 
| Soft soldering with flux | 3 | 
| Gas | 3 | 
| MIG | 1 | 
| Resistance spot welding | 3 | 
| TIG | 2 | 
| welding additives | 
 | 
| Aviation | No | 
| Cr (to) | 0,25 | 
| Cu (to) | 0,1 | 
| Fe (to) | 0,5 | 
| Mg (from) | 0,6 | 
| Mg (to) | 1,2 | 
| Mn (from) | 0,4 | 
| Mn (to) | 1 | 
| Other | 0,05 | 
| Rest | Aluminium | 
| Si (from) | 0,7 | 
| Si (to) | 1,3 | 
| Ti (to) | 0,1 | 
| Total | 0,15 | 
| Zn (to) | 0,2 | 
(a) Includes all listed elements for which no limits are specified. (b) The sum of these "other impurities" whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
| Anodise - decorative | 3 | 
| Anodising - protective anodising | 1 | 
| Normal atmosphere | 1 | 
| Seawater atmosphere | 2 | 
| suitable according to DIN EN 602 | Yes | 
| Bending | 3 | 
| Bending delivery conditions | T3 · T4 | 
| Deep drawing (conditional) | 2 | 
| Deep drawing conditions | O | 
| Drop forging | 2 | 
| Extruding | 2 | 
| Impact extrusion | 2 | 
| Impact extrusion conditions | O | 
| Open die forging | 2 | 
| Press | 2 | 
| Press conditions | O | 
| Upsetting (Conditional) | 2 | 
| Upsetting conditions | O | 
| Heating time max. | 2 h | 
| Heating time min. | 1 h | 
| Annealing temperature max. | 420 °C | 
| Annealing temperature min. | 380 °C | 
| Cooling conditions | ≤ 30°C/h up to 250°C, below 250°C in the air | 
| Cold ageing max. | 8 d | 
| Cold ageing min. | 5 d | 
| Heat ageing max. | 16 h | 
| Heat ageing min. | 4 h | 
| Heating temperature max. | 190 °C | 
| Heating temperature min. | 155 °C | 
| Quenching | Water, Air | 
| Solution annealing max. | 540 °C | 
| Solution annealing min. | 525 °C | 
| dimensional stability | 3 | 
| Eroding | 1 | 
| hardened | 2 | 
| soft annealed | 4 | 
| Colorcode | Enzianblau (RAL 5010) | 
| Material chemically EN 573-3 | AlSi1MgMn | 
| DIN | 3,2315 | 
| DIN (old designation) | Al Mg Si1 | 
| France AFNOR | A-SGM0,7 | 
| Italy UNI | 9006/4 | 
| Material no | EN AW-6082 | 
| Norway | - | 
| Spain | L-3453 | 
| Sweden | 144.212 | 
| United Kingdom BS | H30 | 
| Polishing | 1 | 
| Painting / Coating | 2 | 
| Coefficient of thermal expansion from 20 to 100°C | 23.4 K⁻¹10⁻⁶ | 
| Density | 2.7 g/cm³ | 
| Electrical conductivity max. | 32 m/Ω*mm² | 
| Electrical conductivity min. | 24 m/Ω*mm² | 
| Modulus of elasticity | 70 GPa | 
| Shear modulus | 26.4 GPa | 
| Specific heat | 896 J/(kg·K) | 
| Thermal conductivity max. | 220 W/m*K | 
| Thermal conductivity min. | 170 W/m*K | 
| Brazing | 4 | 
| Brazing with flux | 3 | 
| Friction soldering | 2 | 
| Soft soldering with flux | 3 | 
| Gas | 3 | 
| MIG | 1 | 
| Resistance spot welding | 3 | 
| TIG | 2 | 
| welding additives | 
 | 
| Aviation | No | 
| Cr (to) | 0,25 | 
| Cu (to) | 0,1 | 
| Fe (to) | 0,5 | 
| Mg (from) | 0,6 | 
| Mg (to) | 1,2 | 
| Mn (from) | 0,4 | 
| Mn (to) | 1 | 
| Other | 0,05 | 
| Rest | Aluminium | 
| Si (from) | 0,7 | 
| Si (to) | 1,3 | 
| Ti (to) | 0,1 | 
| Total | 0,15 | 
| Zn (to) | 0,2 | 
(a) Includes all listed elements for which no limits are specified. (b) The sum of these "other impurities" whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
| Anodise - decorative | 3 | 
| Anodising - protective anodising | 1 | 
| Normal atmosphere | 1 | 
| Seawater atmosphere | 2 | 
| suitable according to DIN EN 602 | Yes | 
| Bending | 3 | 
| Bending delivery conditions | T3 · T4 | 
| Deep drawing (conditional) | 2 | 
| Deep drawing conditions | O | 
| Drop forging | 2 | 
| Extruding | 2 | 
| Impact extrusion | 2 | 
| Impact extrusion conditions | O | 
| Open die forging | 2 | 
| Press | 2 | 
| Press conditions | O | 
| Upsetting (Conditional) | 2 | 
| Upsetting conditions | O | 
| Heating time max. | 2 h | 
| Heating time min. | 1 h | 
| Annealing temperature max. | 420 °C | 
| Annealing temperature min. | 380 °C | 
| Cooling conditions | ≤ 30°C/h up to 250°C, below 250°C in the air | 
| Cold ageing max. | 8 d | 
| Cold ageing min. | 5 d | 
| Heat ageing max. | 16 h | 
| Heat ageing min. | 4 h | 
| Heating temperature max. | 190 °C | 
| Heating temperature min. | 155 °C | 
| Quenching | Water, Air | 
| Solution annealing max. | 540 °C | 
| Solution annealing min. | 525 °C | 
| dimensional stability | 3 | 
| Eroding | 1 | 
| hardened | 2 | 
| soft annealed | 4 | 
| Colorcode | Enzianblau (RAL 5010) | 
| Material chemically EN 573-3 | AlSi1MgMn | 
| DIN | 3,2315 | 
| DIN (old designation) | Al Mg Si1 | 
| France AFNOR | A-SGM0,7 | 
| Italy UNI | 9006/4 | 
| Material no | EN AW-6082 | 
| Norway | - | 
| Spain | L-3453 | 
| Sweden | 144.212 | 
| United Kingdom BS | H30 | 
| Polishing | 1 | 
| Painting / Coating | 2 | 
| Coefficient of thermal expansion from 20 to 100°C | 23.4 K⁻¹10⁻⁶ | 
| Density | 2.7 g/cm³ | 
| Electrical conductivity max. | 32 m/Ω*mm² | 
| Electrical conductivity min. | 24 m/Ω*mm² | 
| Modulus of elasticity | 70 GPa | 
| Shear modulus | 26.4 GPa | 
| Specific heat | 896 J/(kg·K) | 
| Thermal conductivity max. | 220 W/m*K | 
| Thermal conductivity min. | 170 W/m*K | 
| Brazing | 4 | 
| Brazing with flux | 3 | 
| Friction soldering | 2 | 
| Soft soldering with flux | 3 | 
| Gas | 3 | 
| MIG | 1 | 
| Resistance spot welding | 3 | 
| TIG | 2 | 
| welding additives | 
 | 
| Aviation | No | 
| Cr (to) | 0,25 | 
| Cu (to) | 0,1 | 
| Fe (to) | 0,5 | 
| Mg (from) | 0,6 | 
| Mg (to) | 1,2 | 
| Mn (from) | 0,4 | 
| Mn (to) | 1 | 
| Other | 0,05 | 
| Rest | Aluminium | 
| Si (from) | 0,7 | 
| Si (to) | 1,3 | 
| Ti (to) | 0,1 | 
| Total | 0,15 | 
| Zn (to) | 0,2 | 
(a) Includes all listed elements for which no limits are specified. (b) The sum of these "other impurities" whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
| Anodise - decorative | 3 | 
| Anodising - protective anodising | 1 | 
| Normal atmosphere | 1 | 
| Seawater atmosphere | 2 | 
| suitable according to DIN EN 602 | Yes | 
| Bending | 3 | 
| Bending delivery conditions | T3 · T4 | 
| Deep drawing (conditional) | 2 | 
| Deep drawing conditions | O | 
| Drop forging | 2 | 
| Extruding | 2 | 
| Impact extrusion | 2 | 
| Impact extrusion conditions | O | 
| Open die forging | 2 | 
| Press | 2 | 
| Press conditions | O | 
| Upsetting (Conditional) | 2 | 
| Upsetting conditions | O | 
| Heating time max. | 2 h | 
| Heating time min. | 1 h | 
| Annealing temperature max. | 420 °C | 
| Annealing temperature min. | 380 °C | 
| Cooling conditions | ≤ 30°C/h up to 250°C, below 250°C in the air | 
| Cold ageing max. | 8 d | 
| Cold ageing min. | 5 d | 
| Heat ageing max. | 16 h | 
| Heat ageing min. | 4 h | 
| Heating temperature max. | 190 °C | 
| Heating temperature min. | 155 °C | 
| Quenching | Water, Air | 
| Solution annealing max. | 540 °C | 
| Solution annealing min. | 525 °C | 
| dimensional stability | 3 | 
| Eroding | 1 | 
| hardened | 2 | 
| soft annealed | 4 | 
| Colorcode | Enzianblau (RAL 5010) | 
| Material chemically EN 573-3 | AlSi1MgMn | 
| DIN | 3,2315 | 
| DIN (old designation) | Al Mg Si1 | 
| France AFNOR | A-SGM0,7 | 
| Italy UNI | 9006/4 | 
| Material no | EN AW-6082 | 
| Norway | - | 
| Spain | L-3453 | 
| Sweden | 144.212 | 
| United Kingdom BS | H30 | 
| Polishing | 1 | 
| Painting / Coating | 2 | 
| Coefficient of thermal expansion from 20 to 100°C | 23.4 K⁻¹10⁻⁶ | 
| Density | 2.7 g/cm³ | 
| Electrical conductivity max. | 32 m/Ω*mm² | 
| Electrical conductivity min. | 24 m/Ω*mm² | 
| Modulus of elasticity | 70 GPa | 
| Shear modulus | 26.4 GPa | 
| Specific heat | 896 J/(kg·K) | 
| Thermal conductivity max. | 220 W/m*K | 
| Thermal conductivity min. | 170 W/m*K | 
| Brazing | 4 | 
| Brazing with flux | 3 | 
| Friction soldering | 2 | 
| Soft soldering with flux | 3 | 
| Gas | 3 | 
| MIG | 1 | 
| Resistance spot welding | 3 | 
| TIG | 2 | 
| welding additives | 
 | 
| Aviation | No | 
| Cr (to) | 0,25 | 
| Cu (to) | 0,1 | 
| Fe (to) | 0,5 | 
| Mg (from) | 0,6 | 
| Mg (to) | 1,2 | 
| Mn (from) | 0,4 | 
| Mn (to) | 1 | 
| Other | 0,05 | 
| Rest | Aluminium | 
| Si (from) | 0,7 | 
| Si (to) | 1,3 | 
| Ti (to) | 0,1 | 
| Total | 0,15 | 
| Zn (to) | 0,2 | 
(a) Includes all listed elements for which no limits are specified. (b) The sum of these "other impurities" whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
| Anodise - decorative | 3 | 
| Anodising - protective anodising | 1 | 
| Normal atmosphere | 1 | 
| Seawater atmosphere | 2 | 
| suitable according to DIN EN 602 | Yes | 
| Bending | 3 | 
| Bending delivery conditions | T3 · T4 | 
| Deep drawing (conditional) | 2 | 
| Deep drawing conditions | O | 
| Drop forging | 2 | 
| Extruding | 2 | 
| Impact extrusion | 2 | 
| Impact extrusion conditions | O | 
| Open die forging | 2 | 
| Press | 2 | 
| Press conditions | O | 
| Upsetting (Conditional) | 2 | 
| Upsetting conditions | O | 
| Heating time max. | 2 h | 
| Heating time min. | 1 h | 
| Annealing temperature max. | 420 °C | 
| Annealing temperature min. | 380 °C | 
| Cooling conditions | ≤ 30°C/h up to 250°C, below 250°C in the air | 
| Cold ageing max. | 8 d | 
| Cold ageing min. | 5 d | 
| Heat ageing max. | 16 h | 
| Heat ageing min. | 4 h | 
| Heating temperature max. | 190 °C | 
| Heating temperature min. | 155 °C | 
| Quenching | Water, Air | 
| Solution annealing max. | 540 °C | 
| Solution annealing min. | 525 °C | 
| dimensional stability | 3 | 
| Eroding | 1 | 
| hardened | 2 | 
| soft annealed | 4 | 
| Colorcode | Enzianblau (RAL 5010) | 
| Material chemically EN 573-3 | AlSi1MgMn | 
| DIN | 3,2315 | 
| DIN (old designation) | Al Mg Si1 | 
| France AFNOR | A-SGM0,7 | 
| Italy UNI | 9006/4 | 
| Material no | EN AW-6082 | 
| Norway | - | 
| Spain | L-3453 | 
| Sweden | 144.212 | 
| United Kingdom BS | H30 | 
| Polishing | 1 | 
| Painting / Coating | 2 | 
| Coefficient of thermal expansion from 20 to 100°C | 23.4 K⁻¹10⁻⁶ | 
| Density | 2.7 g/cm³ | 
| Electrical conductivity max. | 32 m/Ω*mm² | 
| Electrical conductivity min. | 24 m/Ω*mm² | 
| Modulus of elasticity | 70 GPa | 
| Shear modulus | 26.4 GPa | 
| Specific heat | 896 J/(kg·K) | 
| Thermal conductivity max. | 220 W/m*K | 
| Thermal conductivity min. | 170 W/m*K | 
| Brazing | 4 | 
| Brazing with flux | 3 | 
| Friction soldering | 2 | 
| Soft soldering with flux | 3 | 
| Gas | 3 | 
| MIG | 1 | 
| Resistance spot welding | 3 | 
| TIG | 2 | 
| welding additives | 
 | 
                            1 very good
                            2 good
                            3 moderate
                            4 poor
                            5 unsuited
                            0 Not specified