EN AW-5005A
sheet rolled
- Form sheet rolled
- Material Aluminum
- Material EN AW-5005A
- Material chemically EN 573-3 Al Mg1 (C)
- DIN 3.3315
BIKAR Metals companies
Food industry (containers · boxes · packaging)
Building industry (panelling · roofing)
Furniture industry
Refrigeration and air conditioning systems
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
Aviation | No |
Cr (to) | 0.1 |
Cu (to) | 0.05 |
Fe (to) | 0.45 |
Mg (from) | 0.7 |
Mg (to) | 1.1 |
Mn (to) | 0.15 |
Other | 0,05 |
Rest | Aluminium |
Si (to) | 0.3 |
Total | 0,15 |
Zn (to) | 0.2 |
(a) Includes all listed elements for which no limits are given. (b) The sum of these 'other impurities' whose mass fraction is individually 0,010 % or more is expressed with two decimal places before the summation.
Anodise - decorative | 2 |
Anodising - protective anodising | 1 |
Chromating | 2 |
Cleaning / degreasing | 2 |
Hard anodising | 2 |
Phosphating | 2 |
Pickling | 2 |
Shining | 2 |
special anodising quality EQ | 1 |
Normal atmosphere | 1 |
Seawater atmosphere | 2 |
Laser cutting | 3 |
Plasma cutting | 2 |
Sawing | 4 |
Shear cutting | 2 |
Waterjet cutting | 1 |
suitable according to DIN EN 602 | Yes |
Bending | 2 |
Deep drawing (conditional) | 2 |
Deep drawing conditions | O |
Extruding | 2 |
Impact extrusion | 3 |
Press | 3 |
Upsetting (Conditional) | 2 |
Upsetting conditions | O |
Heating time max. | 2 h |
Heating time min. | 1 h |
Annealing temperature max. | 380 °C |
Annealing temperature min. | 360 °C |
Cooling conditions | kiln - uncontrolled |
cold worked | 2 |
Eroding | 1 |
Etching | 2 |
Photo etching | 2 |
soft annealed | 4 |
Material chemically EN 573-3 | Al Mg1 (C) |
DIN | 3.3315 |
DIN (old designation) | Al Mg1 |
France AFNOR | A-G0,6 |
Italy UNI | 9005/1 |
Spain | L-3350 |
Sweden | 144,106 |
United Kingdom BS | N41 |
Blasting | 1 |
Brushing | 3 |
Dessinating | 1 |
Grinding | 3 |
Polishing | 2 |
Galvanising | 2 |
Nickel coating | 1 |
Thermal spraying | 3 |
Enamelling | 2 |
Laminating | 2 |
Painting / Coating | 1 |
Coefficient of thermal expansion from 20 to 100°C | 23.6 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 200°C | 24.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from 20 to 300°C | 25.5 K⁻¹10⁻⁶ |
Coefficient of thermal expansion from -50 to 20°C | 21.8 K⁻¹10⁻⁶ |
Density | 2.69 g/cm³ |
Electrical conductivity max. | 31 m/Ω*mm² |
Electrical conductivity min. | 23 m/Ω*mm² |
Modulus of elasticity | 69.5 GPa |
Shear modulus | 26.1 GPa |
Thermal conductivity max. | 220 W/m*K |
Thermal conductivity min. | 160 W/m*K |
Brazing | 4 |
Brazing with flux | 5 |
Friction soldering | 2 |
Soft soldering | 4 |
Soft soldering with flux | 3 |
Friction stir welding | 2 |
Friction welding | 2 |
Gas | 2 |
Laser | 2 |
MIG | 2 |
Plasma | 2 |
Resistance spot welding | 3 |
TIG | 2 |
welding additives |
|
1 very good
2 good
3 moderate
4 poor
5 unsuited
0 Not specified