CW004A
tube - round as bar
- Form tube - round as bar
- Material Copper
- Material CW004A
- Material chemically EN 573-3 Cu-ETP
BIKAR Metals companies
Windings for motors, generators & transformers
Cables & wires for household, industrial & automotive use
Rail technology: trains, trams, overhead lines
Telecommunications: telephone, signal & submarine cables
Electrical installations: busbars, switches, contacts
Parts for radios, TVs & switchgear
Lightning protection & grounding systems
Electroplating: anodes & plating applications
Coaxial cables & welding electrodes
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
| Aviation | No |
| Bi (from) | 0,0005 |
| Bi (to) | 0,0005 |
| Cu footnote reference | Einschließlich Silber bis max. 0,015 % |
| Other | 0,03 |
| Pb (from) | 0,005 |
| Pb (to) | 0,005 |
| Rest | Cu |
| suitable according to DIN EN 602 | No |
| Material chemically EN 573-3 | Cu-ETP |
| Material no | CW004A (former 2.0065, 2.0060) |
| Coefficient of thermal expansion from 20 to 100°C | 16.8 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 200°C | 17.3 K⁻¹10⁻⁶ |
| Coefficient of thermal expansion from 20 to 300°C | 17.7 K⁻¹10⁻⁶ |
| Density | 8.93 g/cm³ |
| Modulus of elasticity at 100°C | 126 GPa |
| Modulus of elasticity at 20°C | 130 GPa |
| Modulus of elasticity at 200°C | 122 GPa |
| Modulus of elasticity at 300°C | 116 GPa |
| Specific electrical conductivity at 100°C | 43 m/Ω*mm² |
| Specific electrical conductivity at 20°C | 57 m/Ω*mm² |
| Specific electrical conductivity at 200°C | 33 m/Ω*mm² |
| Specific electrical conductivity at -100°C | 110 m/Ω*mm² |
| Specific electrical conductivity at -200°C | 460 m/Ω*mm² |
| Specific electrical resistance at 100°C | 0.023 Ω*mm²/m |
| Specific electrical resistance at 20°C | 0.018 Ω*mm²/m |
| Specific electrical resistance at 200°C | 0.03 Ω*mm²/m |
| Specific electrical resistance at -100°C | 0.009 Ω*mm²/m |
| Specific electrical resistance at -200°C | 0.002 Ω*mm²/m |
| Specific heat at 100°C | 0.393 J/(kg·K) |
| Specific heat at 20°C | 0.386 J/(kg·K) |
| Specific heat at 200°C | 0.403 J/(kg·K) |
| Thermal conductivity at 100°C | 385 W/m*K |
| Thermal conductivity at 20°C | 394 W/m*K |
| Thermal conductivity at 200°C | 381 W/m*K |
| Thermal conductivity at -100°C | 435 W/m*K |
| Thermal conductivity at -200°C | 574 W/m*K |
| Brazing | 2 |
| Soft soldering | 1 |
| Gas | 5 |
| MIG | 5 |
| Resistance spot welding | 5 |
| TIG | 5 |
1 very good
2 good
3 moderate
4 poor
5 unsuited
0 Not specified